Fixed Carbon in Shisha Charcoal: Calculated by Difference, the Intake Limit and Our Measured Value

This page belongs to the quality parameters and shows how the fixed carbon of shisha charcoal, the hookah charcoal or hookah coals of US and Canadian buyers, is worked out on this factory's laboratory report. It is written for the buyer comparing two reports. Fixed carbon is calculated, not weighed.

Written by
Henry Sinaga
Reviewed by
Dimas Setyawan,
Updated
Reading time
4 min read

Quick answer

How is fixed carbon in shisha charcoal worked out, and what does this factory accept?

Fixed carbon is calculated by difference, 100 minus moisture, ash and volatile matter; incoming shell charcoal is accepted at 82% or more. On the newest report on file, issued November 4, 2026, the coconut shell charcoal briquettes measured 82.82% as received: 100 minus 3.21, 1.64 and 12.33. Compare two figures only on the same basis.

Fixed carbon at a glance

As confirmed, November 2026

How it is obtained
Calculated by difference: 100 minus moisture, ash and volatile matter
Intake limit
82% or more, on shell charcoal
Newest report
82.82% as received, November 4, 2026
Check
The four results add up to 100.00%
Grade limit
None; ash alone sets the grade

1. What fixed carbon is

Fixed carbon is the solid carbon left in a sample once everything else has been accounted for.

Definition

fixed carbon

Fixed carbon is the share of a charcoal sample's mass left once moisture, volatile matter and ash are accounted for, calculated by difference as 100 minus those three, in percent on a named basis.

FAO's handbook on charcoal making gives a span for charcoal from about 50% to around 95% fixed carbon. The figure is stated on a reporting basis, like the three results it is calculated from.

How facts on this page are confirmed is set out in the editorial and review policy.

2. Calculated by difference

Fixed carbon is what remains of 100 once moisture, ash and volatile matter are taken away.

ASTM D1762-84 (2021), the method named on this factory's report, covers moisture, volatile matter and ash; fixed carbon is calculated by the laboratory. The register states the method as follows: Carsurin Tbk, Semarang laboratory (KAN accreditation LP-415-IDN for ISO/IEC 17025:2017, as printed on its reports), tests moisture, ash and volatile matter by ASTM D1762-84 (2021), sections 7.2, 7.4 and 7.3, and calculates fixed carbon (method MWI.01.63.LC).

Fixed carbon of the newest laboratory report on this factory's coconut shell charcoal briquettes, issued November 4, 2026, worked from the other three results in percent as received; the result matches the laboratory's own figure.
StepPercent, as received
Start 100.00
Minus moisture − 3.21
Minus ash − 1.64
Minus volatile matter − 12.33
Fixed carbon = 82.82

Because fixed carbon is the remainder, an error in any of the three measured results carries straight into it.

3. The intake limit and our measured value

Shell charcoal is accepted at fixed carbon of 82% or more; the newest report measured 82.82% on finished briquettes.

The intake limit applies to shell charcoal as it arrives from carbonizers, before milling; see how incoming shell charcoal is checked. The report's figure is on finished briquettes, binder included, as received, so the two are not the same measurement.

Results from further shipments are added to the measured fixed carbon of our last batches as they are tested.

4. Comparing fixed carbon figures

Two fixed carbon figures compare only on the same basis and when each report adds up.

  1. Step 1

    Check the basis

    As received or dry. A dry-basis figure is higher than an as-received one for the same charcoal, because the moisture is left out.

  2. Step 2

    Add up the four results

    They should make 100. On a report that calculates fixed carbon by difference, moisture, ash, volatile matter and fixed carbon add up to 100.

  3. Step 3

    Read the moisture beside it

    Wetter means lower. With everything else equal, more moisture as received means less fixed carbon as received.

No grade carries a fixed carbon limit at this factory: the grades page sets each grade by ash alone. How moisture moves the figure is on the moisture content page.

Questions buyers ask

Why is fixed carbon not measured directly?
The method measures moisture, ash and volatile matter, and the laboratory calculates fixed carbon from them by difference. An error in any of the three therefore carries into the fixed carbon figure.
Can I compare your fixed carbon with another supplier's?
Only on the same basis and when the four results on each report add up to 100. A dry-basis figure is higher than an as-received one for the same charcoal, because the moisture is left out.

Sources

  1. ASTM D1762-84(2021), Standard Test Method for Chemical Analysis of Wood Charcoal (the edition named on the laboratory report) (opens in new tab), ASTM International — accessed
  2. Simple technologies for charcoal making (FAO Forestry Paper 41), chapter 10: Using charcoal efficiently (opens in new tab), Food and Agriculture Organization of the United Nations — accessed